TABLE 1

Pilot -scale heap leach test of a low-grade greek nickel oxide ore by the HELLAS Method

Percent extraction of metals

Α/Α

Leach Cycle

Leach Cycle Duration

(days)

ELEMENTS

Fe/Ni

In the leach liquor

Ni recovery

(%)

Co recovery

(%)

Fe recovery

(%)

Al recovery

(%)

Cr recovery

(%)

Mg recovery

(%)

Mn recovery

(%)

0

0

0

0

0

0

0

0

0

0

1

28

21,08

10,63

2,94

3,65

1,19

12,01

31,69

6,51

2

21

31,09

17,59

5,58

6,23

3,06

37,03

32,89

8,75

3

35

40,24

22,41

7,94

5,51

4,46

52,54

39,63

9,61

4

30

51,42

31,20

11,07

7,31

5,88

60,47

45,65

10,50

Final Recovery after washing (%)

59,34

35,67

12,87

26,34

6,88

69,94

52,19

 

 
 
 

TABLE 2

Final analysis of the Pregnant Leach Solution

Metals

Concentration

(g/l)

Ni

3,41

Co

0,17

Fe

35,80

Al

7,31

Cr

0,94

Mg

5,00

Mn

1,12

 
 
 

 

Figure 1: Percent recoveries of Ni, Co, Fe, Al, Cr, Mg and Mn versus time